Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of RAVAMID® B ST BK45 - PA6 - Ravago Group

Material Data Center offers the following functions for RAVAMID® B ST BK45:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Ravamid B datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
Soluble or severely attacked after brief contact.

Please consider the information about the application of the materials.
Processing/Physical Characteristics単位テスト基準
ISO データ
成形収縮率, 平行 1.0 % ISO 294-4, 2577
成形収縮率, 直角 1.1 % ISO 294-4, 2577
機械的特性単位テスト基準
ISO データ
降伏応力 45 MPa ISO 527
破壊応力 35 MPa ISO 527
破壊ひずみ 20 % ISO 527
曲げ弾性率, 23°C 2100 MPa ISO 178
ノッチ付きシャルピー衝撃強さ, +23°C 14 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30゚C 10.5 kJ/m² ISO 179/1eA
ノッチ付きIzod衝撃強さ, +23°C 14 kJ/m² ISO 180/1A
ノッチ付きIzod衝撃強さ 10.5 kJ/m² ISO 180/1A
温度 -23 °C -
熱的特性単位テスト基準
ISO データ
荷重たわみ温度, 1.80 MPa 50 °C ISO 75-1/-2
ビカット軟化温度, B 190 °C ISO 306
1.5mm厚さでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 1.6 mm -
厚さhでの燃焼性 HB class IEC 60695-11-10
試験片の厚さ 3.2 mm -
グローワイヤ燃焼性指数 (GWFI) 650 °C IEC 60695-2-12
GWFI - 試験片の厚さ 2 mm -
その他の特性.単位テスト基準
吸湿率 0.25 % Sim. to ISO 62
密度. 1090 kg/m³ ISO 1183
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 75 °C -
Pre-drying - Time 3 - 4 h -
Processing humidity ≤0.12 % -
樹脂温度 240 - 270 °C -
金型温度 70 - 90 °C -
Zone 1 220 - 230 °C -
Zone 2 230 - 245 °C -
Zone 3 250 - 260 °C -
Nozzle temperature 250 - 260 °C -
Screw speed 50 - 80 rpm -
Back pressure 0.4 - 0.8 MPa -
後硬化時間 6 - 8 MPa -
特殊な特性
成形加工法.
射出成形.
納入形状.
特殊な特性.
高耐衝撃及び耐衝撃改良., 紫外線安定化.
Certifications
Recycled Resin Content
領域別の利用可能性
ヨーロッパ.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com